What Hardness Can Be Tapped — Realistic Limits
Not all hardened steel can be tapped with standard HSS taps. Here are the realistic limits by hardness range:
| Hardness | Tap Grade | Feasibility | Notes |
|---|---|---|---|
| Up to 25 HRC | M2 HSS | ✅ Standard | Normal tapping — no special requirements |
| 25–35 HRC | M35 cobalt | ✅ Possible | Reduce speed 30%. Use sulphurised oil. |
| 35–45 HRC | M42 cobalt | ⚠️ Difficult | Very slow speed. Risk of tap breakage. Short tool life. |
| 45–55 HRC | Solid carbide | ⚠️ Possible with carbide | HSS cannot cut above 45 HRC effectively. |
| Above 55 HRC | Not tappable | ❌ Not feasible | Thread grinding or EDM required. No tap works. |
HSS taps (including M42 cobalt) have practical limits at approximately 45 HRC. Above this, the tap material is not significantly harder than the workpiece — cutting becomes impossible and the tap breaks immediately. If your material is above 45 HRC, tap before heat treatment or use thread grinding.
Tap Grade for Hardened Steel
M42 cobalt (8% Co) is the correct HSS grade for hardened steel tapping:
| Grade | Max Workpiece Hardness | Hot Hardness | Brittleness |
|---|---|---|---|
| M2 HSS | ~25 HRC practical | 400°C | Low — handles interrupted cuts |
| M35 Cobalt | ~35 HRC practical | 600°C | Moderate |
| M42 Cobalt | ~45 HRC practical | 650°C+ | Higher — avoid interrupted cuts |
| Solid carbide | ~55 HRC practical | 900°C+ | Very brittle — requires rigid setup |
M42 cobalt is more brittle than M35 — avoid interrupted cuts and side loads that would break the tap. The setup must be rigid: no runout, no misalignment, no vibration.
Tap Type for Hardened Steel
Forming (fluteless) taps cannot be used in hardened steel — the material does not deform plastically enough to allow displacement. Only cutting taps work above 30 HRC.
For hardened steel blind holes: use spiral flute taps to evacuate chips. For through holes: spiral point taps are faster. Straight flute taps are acceptable for interrupted cuts where the stronger cross-section reduces breakage risk.
Thread rolling (using a thread rolling tap, also called a roll forming tap for steel) can work in soft-to-medium hardened steel if the material has sufficient ductility. Check the material’s elongation specification — below 8% elongation, thread rolling is not feasible.
Tapping Speeds for Hardened Steel
| Material Hardness | M35 Cobalt (m/min) | M42 Cobalt (m/min) | Notes |
|---|---|---|---|
| 25–30 HRC | 8–15 | 10–18 | Use sulphurised oil |
| 30–35 HRC | 5–10 | 8–14 | Reduce speed, flood coolant |
| 35–40 HRC | 3–6 | 5–10 | Very slow — single pass only |
| 40–45 HRC | Not recommended | 3–6 | High breakage risk. Short runs only. |
Coatings That Help in Hardened Steel
TiAlN (titanium aluminium nitride) coating significantly improves tap life in hardened steel by reducing friction and providing a hard, heat-resistant surface:
- TiAlN coating on M42 cobalt taps extends tool life 40–80% in hardened steel by reducing heat transfer to the tap body.
- TiCN coating provides improved hardness (better than TiN) — useful for medium-hardened steel.
- Uncoated M42 is the baseline — suitable when coated taps are not available.
Slugger Tools supplies TiAlN-coated M42 cobalt taps on request for hardened steel applications.
When Tapping Is Not Possible — Alternatives
For material above 45–50 HRC where tapping is not feasible:
- Tap before heat treatment — the most practical solution. Tap the thread in the soft state, then heat treat. Thread may distort slightly but is usually acceptable.
- Thread grinding — CNC thread grinding can produce accurate internal threads in fully hardened material. Slow and expensive but precise.
- EDM (electrical discharge machining) — for very hard materials where no cutting is possible. Slow process.
- Helicoil inserts — tap an oversize hole in the hardened part using a specialised tap, then install a wire thread insert. The insert provides the thread surface.